Solid wood bending processing method with directional bending function
A bending processing and directional bending technology, applied in the direction of wood processing appliances, wood bending, wood heating, etc., can solve the problems of wasting wood, bending or compression parts are not fully softened, wood strength loss, etc., to improve quality, soften The effect of uniform effect and reduced scrap rate
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Benefits of technology
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0031] Embodiment 1: have the solid wood bending processing method of directional bending function, carry out according to the following steps:
[0032] a. Keep the moisture content at 10% and process the naturally dried elm wood to length to make a wood blank with a length of 1m, a width of 0.1m and a height of 0.05m, and determine and mark the position to be bent as the two sides of the middle part of the wood Each extension is 0.25m to form a 0.5m×0.05m×0.1 to be bent part;
[0033] b. Seal and coat the part of the wood blank that does not need to be bent with silicone high-temperature resistant paint so that moisture will not come into contact with the part to be bent;
[0034] c. Soak the sealed wood blank in a water tank until the moisture content of the wood blank to be bent is 30%;
[0035] d. Wrap the wood blank that has absorbed moisture to a predetermined moisture content after soaking with a plastic film, and place it in an incubator at 30°C until the moisture conten
Embodiment 2
[0040] Embodiment 2: the solid wood bending processing method with directional bending function is carried out according to the following steps:
[0041] a. Keep the moisture content at 10% and process the naturally dried elm wood to length to make a wood blank with a length of 1m, a width of 0.1m and a height of 0.05m, and determine and mark the position to be bent as the two sides of the middle part of the wood Each extension of 0.25m forms a 0.5m×0.1m×0.05m to be bent part;
[0042]b. Seal and coat the part of the wood blank that does not need to be bent with silicone high-temperature resistant paint so that moisture will not come into contact with the part to be bent;
[0043] c. Soak the sealed and coated wood blank in a water tank until the moisture content of the wood blank to be bent is 25%;
[0044] d. Wrap the wood blank that has absorbed moisture to a predetermined moisture content after soaking with a plastic film, and place it in an incubator at 50°C until the moist
Embodiment 3
[0049] Embodiment 3: have the solid wood bending processing method of directional bending function, carry out according to the following steps:
[0050] a. Keep the water content at 10% and process the natural dry elm wood to length to make a wood blank, and determine and mark the position to be bent;
[0051] b. Seal and coat the part of the wood blank that does not need to be bent with silicone high-temperature resistant paint so that moisture will not come into contact with the part to be bent;
[0052] c. Soak the sealed wood blank in a water tank until the moisture content of the wood blank to be bent is 25%;
[0053] d. Wrap the wood blank that has absorbed moisture to a predetermined moisture content after soaking with a plastic film, and place it in an incubator at 40°C until the moisture content of the surface layer of the wood blank to be bent and the moisture content of the central layer The difference is less than 5%.
[0054] e. After taking out the wood blank in t
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap